Skip to main content

Table 1 Electrochemical corrosion parameters derived from potentiodynamic polarization curves of the samples. Values are presented as mean ± standard deviation (SD), n = 3

From: Structural optimization of Sr/Zn-phosphate conversion coatings triggered by ions preloading on micro/nanostructured titanium surfaces for bacterial infection control and enhanced osteogenesis

Samples

Ecorr

(V)

Icorr

(×10− 8, A/cm2)

βa

(V·dec− 1)

βc

(V·dec− 1)

Rp

(KΩ·cm2)

M-Ti

-0.50 ± 0.03

41.33 ± 1.90

0.660 ± 0.146

0.127 ± 0.012

110.93 ± 9.31

C-SA

-0.56 ± 0.01

6.47 ± 1.21

0.219 ± 0.003

0.184 ± 0.003

683.78 ± 125.72

C-SLA

-0.48 ± 0.01

2.83 ± 0.11

0.222 ± 0.003

0.184 ± 0.001

1544.34 ± 62.14

C-SLAA

-0.56 ± 0.01

3.36 ± 0.17

0.217 ± 0.003

0.190 ± 0.002

1311.00 ± 67.57

C-IPL

-0.76 ± 0.03

3.66 ± 0.14

0.250 ± 0.003

0.172 ± 0.010

1213.70 ± 81.86